KerfPlot
Measurement units

How to kerf-bend a board (and how deep to cut)

Kerf bending turns a flat board into a curve by sawing a row of slots most of the way through and folding the board around a form. Done by eye it produces flats, cracked skins and open slots. Done with the right numbers it produces a smooth, repeatable curve from ordinary sheet stock.

Updated

Free tool for this guideKerf bendingBend flat stock into a curve without cracking.

How a kerfed board actually bends

Picture the board in cross-section. Each saw cut leaves a thin uncut layer on the far face, called the skin, and a block of solid wood between each pair of cuts (some people call it the pillar or web). When the board bends with the kerfs on the inside of the curve, the wood between cuts rotates about the skin and each slot narrows until its walls meet. The skin is the only part of the board that keeps its original length; it behaves like the pin of a hinge.

That has two consequences for layout. First, kerf spacing must be measured along the hinge arc, the circle that runs through the skin at radius R_h = R_in + d, where d is the kerf depth. Second, every kerf can only rotate until its walls touch, so the number of kerfs is set by how much angle each one can absorb, not by the radius.

Kerf depth
d = T − skin
Hinge radius
R_h = R_in + d
Closing angle per kerf
φ = 2 · atan(K / 2d)
Minimum kerf count
N = ⌈θ / φ⌉
Bend-zone length and spacing
L_h = R_h · θ, S = L_h / N
Wood between cuts
w = S − K

Here T is the stock thickness, K the kerf width, θ the bend angle in radians and R_in the inside radius. The older shop rule of N = d·θ / K, which divides the length the inside face has to lose by the kerf width, usually gives the same count but can ask each slot to close slightly more than it physically can. The closing-angle form is the one KerfPlot uses.

Thin-kerf vs. full-kerf blades

Blade choice changes the kerf count more than any other variable. A wider kerf lets each slot close through a larger angle, so fewer cuts are needed and the wood between them is wider and stronger. A thinner kerf needs more cuts but leaves less visible slot on an exposed inside face. The table holds the stock and curve constant: 3/4" plywood with a 3/32" skin, a 12" inside radius and a 90° bend.

BladeKerf Kφ per kerfCuts NSpacing SWood between cuts
Thin-kerf table saw3/32" (2.38 mm)8.17°121.657"1.563"
Full-kerf table saw1/8" (3.18 mm)10.88°92.209"2.084"
Sliding table saw3.5 mm (0.138")11.99°82.485"2.347"
3/4" plywood, 3/32" skin (d = 21/32"), 12" inside radius, 90° bend (L_h = 19.88")

Notice that the number of cuts depends only on blade, depth and bend angle. Keep the full-kerf blade and 90° bend but change the radius, and the count stays at nine while the spacing scales with the hinge arc.

Inside radiusHinge arc L_hCuts NSpacing SWood between cuts
4"7.314"90.813"0.688"
8"13.597"91.511"1.386"
12"19.880"92.209"2.084"
24"38.730"94.303"4.178"
Same stock and 1/8" blade, 90° bend, varying inside radius

The tight-radius limit is therefore not the kerf count. It is the skin: the outside face of a 4" radius bend is stretched far more per inch than the same face on a 24" radius, and thin skins crack across the grain. Thin wood between cuts also becomes fragile and can shear off during clamping. Measure your real kerf with a caliper before trusting any of these numbers; a blade with heavy set or runout cuts wider than its nominal width.

Birch ply, MDF and solid wood: run test strips

The geometry is the same for every material, but the skin is not. Before cutting the real part, cut a test strip about 2" wide and 12" long from the same sheet, with five kerfs at the computed depth and spacing, and bend it over the form.

MaterialSkin to start withKerf directionTypical failure
Baltic / birch plywoodFace veneer plus one cross-plyAcross the face grainCross-ply splits if the skin is only the face veneer.
MDF1/8" (3 mm) or moreAny directionSkin snaps cleanly; fibers have no length to share the load.
Solid straight-grained hardwood1/8" or moreAcross the grain onlySplits along runout or knots near the skin.
Bending plywood (lauan or poplar)Usually not kerfedn/aAlready bends to tight radii without kerfs in the long-grain direction.
How common materials behave as a kerf skin
  • Kerfs close before the strip reaches the form: the slots are too narrow for the bend. Add a cut or use a wider blade.
  • The strip touches the form but slots gape and show flats: spacing is too wide. Recompute with more cuts.
  • The skin cracks: leave more skin, increase the radius, or lightly dampen the outside face (never the kerfed face) before bending.
  • The wood between cuts snaps off: it is too thin. Use a wider blade so fewer, wider blocks carry the bend.

Set blade height with a test cut in scrap and measure the remaining skin with a caliper. On a table saw, a 1/64" change in blade height is a 17% change in a 3/32" skin, so creep up on the setting rather than reading it from the height scale.

Building the clamping form

A kerfed board bends against a male (convex) form with the kerfed face touching it. Build the form from two or three layers of 3/4" MDF or plywood cut to the inside radius and glued face to face, so it is at least as wide as the workpiece. A printed 1:1 arc template makes the form layout as accurate as the part.

  1. Cut the form 1/16" outside the line on the bandsaw, then fair it to the line with a spokeshave, rasp or disc sander. Flats on the form become flats on the part.
  2. Add straight lead-ins tangent to the curve so the flat ends of the blank have somewhere to land.
  3. Wax the form or cover it in packing tape so squeeze-out does not glue the part to it.
  4. Pull the board around with a ratchet strap or band clamp, or use a matching female caul cut from the same template, offset by the stock thickness.
  5. Work from one end: clamp the first lead-in flat, then wrap progressively so each kerf closes in turn.

Locking the curve: epoxy, PVA and backers

A kerfed board on its own springs back toward flat when it comes off the form. Something has to fix the wood between cuts in place. Glue the kerfs only after the board is wrapped on the form and the slots have closed to their final width; glue put in first lubricates the slots and lets the board slide.

MethodStrengthGap toleranceNotes
Epoxy thickened with wood flourHighFills open kerfs fullyLong open time suits slow wrapping; tint matches the wood.
PVA wood glueGood on tight jointsPoor; not a gap fillerUse only where kerfs close completely; clamp time is short.
Laminated backer veneer or bending plyHigh, and stiffens the curveBridges open kerfsGlue to the kerfed face on the form; hides the slots entirely.
Glue blocks or a rib frameDepends on spacingNot neededFor hidden faces such as speaker cabinets and bow-front aprons.
Options for fixing a kerf bend

For a painted part, thickened epoxy or a bending-ply backer gives the most rigid result. For a clear-finished show face on the outside, the kerfs are hidden anyway; for an exposed inside face, a thin-kerf blade and a laminated veneer is the cleanest combination.

Questions from the shop

Do the kerfs go on the inside or the outside of the curve?

The inside (concave) face, against the form. The kerfs close as the board bends. Kerfs on the outside would open, and the skin would have to compress, which wood resists.

Can I kerf bend across the grain of solid wood?

Yes, that is the normal direction: kerfs run across the grain so the skin bends along its long fibers. Kerfing parallel to the grain leaves a skin that splits along the fibers almost immediately.

Why is my curve faceted even though every kerf closed?

The spacing was too wide for the radius, so each block between cuts is a visible flat. More, closer kerfs, or a backer veneer that fairs the curve, will smooth it.

More in Curves and bending